>> 自然科学版 >> 当期目录 >> 力学•土木•材料 >> 正文
陶瓷-钢渣阻热耐磨型沥青混合料路用性能研究
时间: 2026-11-20 次数:

谭波,张婉贞,陈平,等.陶瓷-钢渣阻热耐磨型沥青混合料路用性能研究[J].河南理工大学学报(自然科学版),2027,46(1):173-179.

Tan B, Zhang W Z, Chen P,et al.Road performance of heat-shielding and wear-resistant ceramic-steel slag asphalt mixtures[J].Journal of Henan Polytechnic University(Natural Science) ,2027,46(1):173-179.

陶瓷-钢渣阻热耐磨型沥青混合料路用性能研究

谭波1,2, 张婉贞1,2, 陈平1,2, 黄超旺3, 陈祖洪3

1.桂林理工大学 广西绿色建材与建筑工业化重点实验室,广西 桂林  541004;2.桂林理工大学 土木工程学院,广西 桂林  541004;3.广西壮族自治区 苍梧公路养护中心,广西 梧州  543100

摘要: 目的  针对高温地区重载重交通的二级公路出现的路面病害,制备一种陶瓷-钢渣阻热耐磨型沥青混合料,并对其路用性能进行研究。 方法  将粒径[4.75,9.5] mm的陶瓷和钢渣以等体积方式替代同档石灰岩集料的40%,陶瓷和钢渣的体积比分别设置为2∶2,1∶3,3∶1。通过冻融劈裂试验、车辙试验评价该混合料的水稳定性和高温稳定性,通过室内光照辐射试验和加速磨耗试验验证混合料的阻热性能和耐磨性能。 结果 结果表明:陶瓷和钢渣的加入导致混合料的沥青用量增加,且陶瓷-钢渣沥青混合料的水稳定性和抗车辙性能均有不同程度提高;陶瓷-钢渣沥青混合料降温效果显著,但长时间高温照射也会使上表面温度增加,且二者掺量为2∶2时,4 cm面层的最大温差为5.9 ℃,阻热效果最好;钢渣强度高,表面粗糙度多孔,与沥青结合牢固,其掺量对耐磨性能的影响较大,且随着钢渣掺量增加,耐磨性能显著提高,当钢渣掺量为30%时,混合料在加速磨耗试验中的质量损失最低,为227.1 g,耐磨性能相比于常规纯石灰岩沥青混合料提高了25.10%。 结论  掺量不同,沥青混合料性能变化规律不同,建议陶瓷-钢渣掺量比例控制在2∶2左右,此时沥青混合料综合性能最优,且便于施工配料。

关键词:陶瓷;钢渣;沥青混合料;阻热性能;耐磨性能

doi:10.16186/j.cnki.1673-9787.2024080016

基金项目:国家自然科学基金资助项目(552062009);广西重点研发计划项目(桂科AB23026071)

收稿日期:2024/08/11

修回日期:2024/10/23

出版日期:2026/11/20

Road performance of heat-shielding and wear-resistant ceramic-steel slag asphalt mixtures

Tan Bo1,2, Zhang Wanzhen1,2, Chen Ping1,2, Huang Chaowang3, Chen Zuhong3

1.Guangxi Key Laboratory of Green Building Materials and Construction Industrialization, Guilin University of Technology, Guilin  541004, Guangxi, China;2.School of Civil Engineering, Guilin University of Technology, Guilin  541004, Guangxi, China;3.Cangwu Highway Maintenance Center, Guangxi Zhuang Autonomous Region, Wuzhou  543100, Guangxi, China

Abstract: Objectives A heat-shielding and wear-resistant ceramic-steel slag asphalt mixture was developed to mitigate pavement distress on secondary highways subjected to heavy traffic and high temperatures, and its pavement performance was investigated. Methods  Ceramic and steel slag with particle sizes of 4.75-9.5 mm were used to replace 40% by volume of the limestone aggregate in the corresponding size fraction. The ceramic-to-steel-slag volume ratios were set at 2∶2, 1∶3, and 3∶1. The moisture stability and rutting resistance of the mixtures were evaluated using freeze-thaw splitting and rutting tests, respectively, while their heat-shielding performance and wear resistance were evaluated through indoor light-radiation and accelerated wear tests, respectively. Results  The incorporation of ceramic and steel slag increased the asphalt content of the mixtures and improved their moisture stability and rutting resistance to varying degrees. The ceramic-steel slag asphalt mixtures exhibited a significant cooling effect; however, prolonged exposure to high temperatures also increased the surface temperature. At a ceramic-to-steel-slag ratio of 2∶2, the maximum temperature difference for the 4-cm-thick surface layer was 5.9°C, indicating the best heat-shielding performance. Steel slag exhibited high strength and a rough, porous surface, resulting in strong adhesion to asphalt. The steel slag content had a pronounced effect on wear resistance, which improved progressively with increasing steel slag content. When the steel slag content was 30%, the mixture exhibited the lowest mass loss, 227.1 g, in the accelerated wear test, representing a 25.10% improvement in wear resistance compared with the conventional limestone-only asphalt mixture. Conclusions The performance of the asphalt mixtures varied with the ceramic-to-steel-slag ratio. A ratio of approximately 2∶2 is recommended because it provides a favorable balance of overall performance while facilitating construction and material proportioning.

Key words:ceramic;steel slag;asphalt mixture;heat-shielding performance;wear resistance